Written by the Popper tooling team We build and run production molds in Foshan and see these defects on real trials every week. The notes below are the ones we send back to customers when a sample comes out wrong. Last reviewed: 2026-11-26
Two injection mold halves resting on a workbench, guide pins and cavities visible
Most defects are decided here, on the bench, before the tool ever reaches a press. This is also where they are cheapest to fix.

The defect is rarely one person's fault

A sink mark can come from a thick section, a cold mold, a short pack phase or a gate in the wrong place. That is four owners for one blemish, and it is why the defect conversation turns into a blame loop so fast. The useful way to run it is to change one variable and see what moves. Everything else is argument.

Before we get into each defect, the ground rules. If you are buying a mold, you want the part right. Your mold maker wants the part right too, because re-cutting steel on his side costs more than re-running the trial. When a defect shows up at T1, the fastest path is a clear description and the settings, not a demand to "fix the tool". The fix might be in the resin, the machine or the drawing.

This article fits between what T1 samples actually tell you and the DFM review that prevents most of these in the first place. If you are still comparing quotes, start with what drives mold cost.

The short list at a glance

DefectWhat you seeMost common causeUsually fixed in
Short shotPart incomplete, missing edgesMaterial froze too early or shot too smallProcess / gate / vent
Sink markDimple on a flat surfaceThick section shrinking as it coolsDesign / gate
Weld lineHairline where flow fronts metTwo fronts meeting around a featureDesign / gate position
WarpagePart bends or twists after ejectionUneven cooling or unbalanced flowDesign / cooling
FlashThin extra material at the parting lineClamp force or worn parting lineProcess / tool
SplaySilver streaks radiating from the gateMoisture or degraded materialMaterial / process
Burn markDark or scorched spotTrapped gas compressingVenting / process

Keep this table near the press. It saves the first hour of every defect conversation.

Short shots

The cavity did not fill. The part comes out with a rounded or missing corner, usually at the far end from the gate. The material set before it reached the end of the flow path, or there simply was not enough of it.

Check in this order: shot size first, then melt temperature and injection speed, then gate size, then venting. A cold tool or a barrel that is not fully up to temperature mimics a short shot, so give the machine time to stabilise before you judge the mold. If the same tool shorts on two different machines, the gate or the wall thickness is the problem.

Thin walls are the usual design cause. If your wall is thinner than the resin can fill before it freezes, no amount of pressure fixes it. This is exactly the kind of thing the wall thickness rules are there to catch early.

Sink marks

A sink mark is a shallow dimple, usually on a flat face, right where a rib or boss attaches on the other side. The thick section under the surface cools slowly and shrinks, and the surface gets pulled down into the gap.

You can mask it by holding pack pressure longer, but that treats the symptom. The fix is to thin the section: core out the thick area, turn a solid boss into a hollow one, or run ribs at about 60 percent of the wall thickness. Moving the gate closer to the thick section also lets it pack before the surrounding skin freezes off.

If a supplier tells you sink marks are "normal for this material", get a second opinion. They are normal for a design that has not been reviewed, which is a different thing.

Weld lines

Weld lines look like a hairline crack or a faint line where two flow fronts met. They appear around holes, bosses and ribs, or anywhere the flow splits and rejoins. They are not cracks in the usual sense, but they are the weakest point in the part and they show up on painted or textured surfaces.

You usually cannot remove them, so you manage them. Raise the melt and mold temperature so the fronts meet while they are still hot enough to fuse. Move the gate so the join lands on a hidden edge. For a cosmetic part, run a flow study before the tool is cut and pick the gate location that pushes the weld line off the show face. Steel selection matters less here than you would think; the gate and the flow path do the work.

Warpage

The part comes out straight and then bends as it cools on the bench. That is warpage. It is the result of the part cooling at different rates in different places, or of internal stress from unbalanced flow being released after ejection.

The common fixes are even wall thickness, balanced cooling lines, and a gate that fills the cavity evenly. Fiber-filled materials warp directionally because the fibers align along the flow, so the gate position and the fiber orientation both matter. If the drawing has a flatness callout, tell the mold maker up front, because that single number can change the gate, the cooling and the tool cost.

Flash

Flash is a thin skirt of extra plastic squeezed out at the parting line. A little of it is a nuisance; a lot of it means the tool is not closing square, the clamp is under-rated for the projected area, or the parting line is worn or dirty.

New tool: check the clamp force against the projected area before you blame the mold. Old tool: look for a battered parting line or a bent plate. Flash on a brand-new tool with correct clamp usually points to the tool not being spotted in properly, which is a toolmaker's job to correct. Our note on hot runner maintenance covers the related problem of leaks at the hot half, which buyers often confuse with parting-line flash.

Splay and burn marks

Splay is a fan of silver or milky streaks radiating from the gate. Burn marks are dark scorched patches, often at the end of the flow path or at a weld line. They look unrelated but share a cause: something is wrong with what is entering the cavity.

Splay is usually moisture or degraded material. Dry the resin properly and check the barrel temperature. Burn marks are trapped air or gas that cannot escape, so the fix is venting: add or clean vents at the end of the flow path, and slow the injection so the gas has time to get out. Scorch marks are also how you spot a barrel that is running too hot and cooking the material.

How to hand a defect to your mold maker

When a sample is wrong, send four things and the problem usually solves itself in one reply. A photo with the defect marked. The gate location and part orientation. The full machine settings. The material grade and lot. A one-line note on when it started beats a paragraph of theory.

We ask for those four things on every trial because they separate design problems from process problems in minutes. If you want this review before the tool is cut, the RFQ checklist and the DFM guide cover what to include, and steel selection covers the material half of the conversation. When a drawing is ready, send it over and we will walk the defect risks with you before quoting.

Have a sample with a defect you cannot name? Send the photo, settings and material.

Get a tooling review →

See the cycle that creates these

Bill Hammack's public explainer on injection molding shows how melt flows, how fronts meet and how the part cools, which is the physics behind most of this list. It is an independent educational video from The Engineer Guy channel, not supplier marketing. Source: YouTube.

Plastic injection molding explainer video
Plastic Injection Molding · The Engineer Guy · external educational source

Frequently asked questions

Sink marks happen where a thick section cools and shrinks more than the thin walls around it. The surface gets pulled inward as the inside solidifies last. The fix is usually to core out the thick section, add ribs instead of a solid block, or move the gate so the part packs before the thin areas freeze off. Pushing up pack pressure and hold time hides it a bit, but it does not remove the root cause.

Weld lines form where two flow fronts meet, usually around a hole, a gate split, or a thin rib. You rarely remove them entirely. You move them somewhere they do not show, or you make the fronts meet hotter and faster. Raising melt temperature, adding a flow leader, or moving the gate so the fronts join at a less visible edge all help. A flow study before cutting steel is the cheap way to find out where they will land.

The cavity did not fill. That means the material froze before it reached the far end, the shot size is short, the gate is too small, or the part is too thin for the resin and machine. It can also be a blocked vent stopping the air from escaping. Start with the shot size and the barrel, then look at gate size and venting before you touch the tool.

Change one thing at a time. Run the same tool on a different machine, or the same machine with a different batch of resin. If the defect follows the tool, it is the tool. If it follows the machine settings, it is the process. If it shows up on every machine and every setting, look at the part geometry. Most shops work through exactly this order before they reach for the grinder.

Four things: a clear photo with the defect circled, the part orientation and gate location marked, the full machine settings (melt temp, mold temp, fill speed, pack and hold pressure), and the material grade with its lot. A short description of when it started helps more than a paragraph of speculation. With those we can usually name the cause in one reply instead of three.

Yes, if you catch them before signing off the design. Weld lines, sink marks, warpage and short shots are almost always cheaper to fix on paper with a flow and cooling study than to correct on a hardened tool. Once the tool is cut and hardened, most corrections mean welding, re-machining or inserts, and none of those are free. This is the whole reason the DFM step exists.

Edited by Jimmy Y. · Popper Tooling Team, Foshan · Last reviewed 2026-11-26